As for the heat treatment for CCS Grade DH36 angle steel, the delivery condition must be Normalized or Normalized rolled or TMCP.
Chemical Composition of CCS DH36 Angle Steel
Grade | C max | Si max | Mn | P max | S max | Als min | Ti max | Cu max | Cr max |
Ni max |
Mo max |
Nb | V |
CCS DH36 | 0.18 | 0.50 | 0.90-1.60 | 0.035 | 0.035 | 0.015 | 0.02 | 0.35 | 0.20 | 0.40 | 0.08 | 0.02-0.05 | 0.05-0.10 |
Ceq% =(C+Mn)/6+(Cr+Mo+V)/5+(Ni+Cu)/15.
CCS DH36, BV/DH36 CCS DH36Z15, CCS DH36Z25,CCS DH36Z35
Mechanical Properties of CCS DH36 Angle Steel
The CCS DH36 angle steelhasyield strength of 335 MPa, and ultimate tensile strength of 490-630 MPa. All the CCS DH36shipbuilding steel offered by Katalor Shanghaican be certificated by China Classification Society (CCS).Grade | Rm (MPa) |
Re(MPa) min | A% min | Akv/J min | ||||||
E.T °C | Thickness (mm) | |||||||||
≤ 50 | >50-70 | >70-100 | ||||||||
L | C | L | C | L | C | |||||
CCS DH36 | 490-630 | 355 | 21 | -40 | 34 | 24 | 41 | 27 | 50 | 34 |
Delivery Condition of CCS DH36 Angle Steel
Grade | Fine grains elements | category | The thickness of steel | ||||||
≤ 12 | >12.5-20 | >20-25 | >25-35 | >35-50 | >50-100 | ||||
DH36 | Any | Plate/sheet | N,TM | ||||||
Profile steel | N(25),TM(25),AR*(15),CR*(15) | - |